# Heat treating 1095

> 1095 knife heat treatment with Celsius and Fahrenheit setpoints, hold times, quench and temper details, equipment assumptions and workshop checks.

Source: https://knifetemplates.com/heat-treating/1095

[Learn](https://knifetemplates.com/guides) / [Heat treating](https://knifetemplates.com/heat-treating)

1095 is familiar, but I would not pick it just because the name sounds simple. The quick transfer and fast quench deserve as much attention as the temperature on the furnace.

[Knife Templates](https://knifetemplates.com/makers/knife-templates) · 5 min read

## Where I would start

A non-stainless option for makers who want a carbon-steel blade and already have a controlled process. A hamon project adds another set of variables; the through-hardening route here does not describe clay coating or water quenching.

Known annealed 1095 bar, stock removal, controlled furnace and a through-hardening oil quench. Check the material supplier and batch before treating 1095 as interchangeable with another bar.

## Get the equipment ready

A controlled furnace, compatible anti-scale coating, fast commercial quench oil and a verified tempering oven. Arrange a short, clear transfer to the tank.

Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.

## A process to work from

Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.

*1095: worked heat-treatment route*

| Stage | What to do |
| --- | --- |
| Prepare | Drill, deburr and inspect the blank. Set the furnace, oil and tempering oven up before loading. |
| Austenitise | Example: 802°C / 1475°F. Hold 10 minutes after equalisation, within the supplier’s 5–15 minute window for section and equipment. |
| Quench | Use Parks 50 with a prompt, controlled transfer. A slower oil can leave inadequate hardness. Water or brine is not part of this route. |
| Temper | At near room temperature, begin 204°C / 400°F for 2 hours. Cool to room temperature and repeat for 2 hours. |
| Check | Remove decarburised material at the test site before judging the hardness. Check several positions on a representative coupon. |

### Before the blade gets hot

Have the tempering setup ready. Oil quenching needs a stable non-combustible tank, sufficient depth and volume, a fitted metal lid, ventilation and suitable fire protection. Keep water away from quench oil. Never use waste motor oil.

### How far to trust this route

This 1095 route follows New Jersey Steel Baron's published sheet for annealed bar, and its numbers match that sheet. Independent testing advises caution with that supplier's datasheets: many of them seem to carry the same recommendations regardless of the steel, and the advice is to avoid them. Reading the 1084, 1095 and O1 sheets (that supplier's O1 sheet is among them) side by side, their tempering hardness tables are identical wherever they overlap, and all four carbon steel sheets carry the same three-step normalising block, which fits what the independent testing describes. I looked for the steel producers' own heat treatment figures for 1084 and 1095 and found none. The only non-retail table I found, a furnace maker's reference (SECO/WARWICK's Heat Treating Data Book), gives a hardening range of 1575 to 1625°F for both, about 100°F hotter than this route, and no tempering temperature. I have kept the route because it is a complete, self-consistent starting point for a coupon. Cross-check it against the steel producer's own datasheet before you rely on any figure.

## The detail to pay attention to

A blade can appear hard in one place and still have an underhardened area elsewhere. Before raising the furnace temperature, check the transfer, actual blade temperature, oil condition, section thickness and whether you are testing through decarb.

Rehearse the transfer with a cold blank and the furnace off. Make sure the tongs hold securely without a change of grip. A hurried turn around a crowded bench is a poor way to save a second. Keep the process recorded so a successful blade can be repeated.

## Check the result before fitting the handle

Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.

Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.

## Keep a record

Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.

After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.

## Where this comes from

- [1095 Heat Treat, July 2020](https://cdn.newjerseysteelbaron.com/wp-content/uploads/2020/07/1095-Heat-Treat-7-20.pdf), New Jersey Steel Baron. Supplier schedule for controlled equipment. Fahrenheit is authoritative where the PDF prints an inconsistent Celsius conversion. Example setpoints below sit inside its ranges; no hardness is guaranteed.
- [Heat Treating Data Book, tenth edition, Table 2](https://www.secowarwick.com/wp-content/uploads/2017/03/HeatTreatingDataEBook.2011.pdf), SECO/WARWICK. A furnace maker’s reference table of heat treating grades of carbon steels, compiled from sources it believes reliable. It is not a steel producer. It gives a hardening range for 1084 and 1095 but no tempering temperature.

[Next up Heat treating 80CrV2 80CrV2: the equipment, hardening hold, quench, temper and details that are easy to miss.](https://knifetemplates.com/heat-treating/80crv2)

## Keep reading

- [Knife steel: 1095](https://knifetemplates.com/steel/1095)
- [Austenitising a knife: temperature and soak](https://knifetemplates.com/heat-treating/austenitising)
- [Quenching knives: oils, plates and speed](https://knifetemplates.com/heat-treating/quenching)
- [Tempering knife steel: temperature and cycles](https://knifetemplates.com/heat-treating/tempering)
- [How to heat treat a knife](https://knifetemplates.com/heat-treating)
- [All heat treating pages](https://knifetemplates.com/heat-treating)

## Put it into practice

[Choose a template](https://knifetemplates.com/templates) [Read the print guide](https://knifetemplates.com/guides/print-at-actual-size) [Arrange blanks on stock](https://knifetemplates.com/nest)