# Heat treating 5160

> 5160 knife heat treatment with Celsius and Fahrenheit setpoints, hold times, quench and temper details, equipment assumptions and workshop checks.

Source: https://knifetemplates.com/heat-treating/5160

[Learn](https://knifetemplates.com/guides) / [Heat treating](https://knifetemplates.com/heat-treating)

5160 often comes up when makers talk about tough working blades. I would start with identified bar and a repeatable schedule rather than an unknown spring with years of service behind it.

[Knife Templates](https://knifetemplates.com/makers/knife-templates) · 4 min read

## Where I would start

A non-stainless spring steel commonly considered for larger working knives. Thickness and edge geometry still decide much of how a finished blade cuts and survives use.

Annealed stock-removal material using the NJSB supplier route below. This is separate from the frequently quoted cryogenic toughness experiments on forged, normalised and annealed specimens.

## Get the equipment ready

A controlled furnace, anti-scale protection, medium-speed commercial oil such as Parks AAA, and a verified tempering oven.

Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.

## A process to work from

Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.

*5160: worked heat-treatment route*

| Stage | What to do |
| --- | --- |
| Austenitise | Example: 802°C / 1475°F, inside the supplier’s 1465–1480°F window. Hold 10 minutes after equalisation, within its 5–15 minute allowance for section and equipment. |
| Quench | Use the supplier’s medium-speed oil route, for example Parks AAA, operated to the oil maker’s instructions. |
| Temper | Near room temperature, begin 204°C / 400°F for 2 hours. Cool to room temperature and repeat for 2 hours. |
| Cold treatment | None specified in this supplier route. Do not attach hardness or toughness figures from a cryogenic experiment to this process. |

### Before the blade gets hot

Have the tempering setup ready. Oil quenching needs a stable non-combustible tank, sufficient depth and volume, a fitted metal lid, ventilation and suitable fire protection. Keep water away from quench oil. Never use waste motor oil.

### How far to trust this route

This 5160 route follows New Jersey Steel Baron's published sheet for annealed bar, and its numbers match that sheet. Independent testing advises caution with that supplier's datasheets: many of them seem to carry the same recommendations regardless of the steel, and the advice is to avoid them. The independent testing of 5160 found a different best window (austenitising at 1500 to 1525°F and tempering at 375 to 400°F, with a liquid nitrogen step), so do not mix the two. I have kept the route because it is a complete, self-consistent starting point for a coupon. Cross-check it against the steel producer's own datasheet before you rely on any figure.

## The detail to pay attention to

You will also find 1500–1525°F recommendations. Those can belong to a different tested process. Keep the prior treatment, oil, cold step and temper with the schedule they came from instead of taking the hottest number from each.

If using forged material, establish its normalising and annealing route before using a stock-removal schedule. If you cannot identify a recycled spring, treat it as an experimental material rather than stamp 5160 on the finished knife. Cracks from prior service are another uncertainty you do not need on an early build.

## Check the result before fitting the handle

Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.

Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.

## Keep a record

Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.

After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.

## Where this comes from

- [5160 Heat Treat, July 2020](https://cdn.newjerseysteelbaron.com/wp-content/uploads/2020/07/5160-Heat-Treat-7-20.pdf), New Jersey Steel Baron. Supplier schedule for controlled equipment. Fahrenheit is authoritative where the PDF prints an inconsistent Celsius conversion. Example setpoints below sit inside its ranges; no hardness is guaranteed.

[Next up Heat treating 52100 52100: the equipment, hardening hold, quench, temper and details that are easy to miss.](https://knifetemplates.com/heat-treating/52100)

## Keep reading

- [Knife steel: 5160](https://knifetemplates.com/steel/5160)
- [Normalising and thermal cycling](https://knifetemplates.com/heat-treating/normalising)
- [Austenitising a knife: temperature and soak](https://knifetemplates.com/heat-treating/austenitising)
- [Quenching knives: oils, plates and speed](https://knifetemplates.com/heat-treating/quenching)
- [Tempering knife steel: temperature and cycles](https://knifetemplates.com/heat-treating/tempering)
- [How to heat treat a knife](https://knifetemplates.com/heat-treating)
- [All heat treating pages](https://knifetemplates.com/heat-treating)

## Put it into practice

[Choose a template](https://knifetemplates.com/templates) [Read the print guide](https://knifetemplates.com/guides/print-at-actual-size) [Arrange blanks on stock](https://knifetemplates.com/nest)