What it is
O1 was the first oil hardening steel, developed in 1905. It is a non-stainless tool steel, and being sold as ground flat stock does not mean it arrives ready to hold an edge.
| Element | Content |
|---|---|
| Carbon | 0.95% |
| Silicon | 0.3% |
| Manganese | 1.1% |
| Chromium | 0.6% |
| Tungsten | 0.55% |
| Vanadium | 0.1% |
What the sources say
The toughness finding is the same as for 1095: O1 and 1095 both showed relatively low toughness in earlier testing, likely because of plate martensite, and the testing favours 52100 over 1095 or O1. In forge heat treating, O1 sits with the fine-cutting steels.
The producers are unusually consistent about this one. Uddeholm, BÖHLER, Industeel and Carpenter all publish a sheet for it, and each gives the standard grade: AISI O1, 1.2510. They agree on an oil quench and a hardening heat between 780 and 850°C. Uddeholm’s table trades time for temperature: 30 minutes at 800°C, 20 at 825°C and 15 at 850°C.
Where to be careful
The sheets differ on the details, so use one complete sheet and keep its numbers together: the route page sets the four side by side. Uddeholm gives its tempering as a graph, which is why the route has a 180°C floor and no single tempering temperature. A supplier's sheet, New Jersey Steel Baron's, says "Parks 50 is not recommended"; none of the four producers names an oil brand.
Where this comes from
- Bainite Heat Treatments of 52100, O1, and 1095: How Much Toughness?, Knife Steel Nerds. Austempering experiments and what they say about plate martensite in 1095 and O1. A different route from quench and temper.
- How to Pick the Best Steel for Every Knife, Knife Steel Nerds. Larrin Thomas’s method for choosing a steel, with his own recommendations. Opinion informed by his testing; the charts are images.
- How to Heat Treat Knife Steel in a Forge, Knife Steel Nerds. A method for reducing forge error, tested on seven low alloy steels. The author still recommends a furnace or a professional for most people.
- Uddeholm Arne data sheet, edition 11, 04.2019, Uddeholm. The producer’s own sheet for an oil-hardening tool steel it lists as “AISI O1, W.-Nr 1.2510”. Producer data. Tempering is given as a graph, so no tempering hardness is quoted here.
- BÖHLER K460 data sheet, BÖHLER (voestalpine). The producer’s own sheet. It says K460 “corresponds to the material 1.2510 (100MnCrW4, O1)”. Producer data; the tempering chart is a graph.
- O1-2510 data sheet, July 2023, Industeel (ArcelorMittal). The producer’s own sheet for AISI O1, W 1.2510. Producer data; the tempering curve is a graph.
- CarTech O1 data sheet, Carpenter Technology. The producer’s own sheet for AISI Type O1. Its tempering chart is linked from the PDF, not in it, so no tempering temperatures are taken from it.
Comments
Questions, corrections and what worked for you. Upvote comments you find useful.