Where I would start
A non-stainless candidate for outdoor and general-purpose blades. Plan the edge for the work it will see; the steel name does not turn a thin kitchen grind into a chopping edge.
Annealed stock-removal bar in a controlled furnace. The 10-minute hold below is for roughly 3.2 mm / 1⁄8 inch stock. Coarse spheroidised material can respond differently; this is not a forge colour-based method.
Get the equipment ready
A controlled furnace, surface protection, commercial quench oil suitable for the stock and section, and a checked tempering oven.
Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.
A process to work from
Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.
| Stage | What to do |
|---|---|
| Austenitise | 829°C / 1525°F for 10 minutes after equalisation at approximately 3.2 mm / 1⁄8 inch thickness. Thicker material needs its own validated hold; 18 minutes was used in the published 6.4 mm / 1⁄4 inch quench experiments. |
| Quench | Oil quench promptly. Medium hardenability permits a wider oil choice than 1095, but starting structure and thickness still matter. |
| Temper | A practical starting point is 204°C / 400°F, two cycles of 2 hours with room-temperature cooling between. Choose the final temperature from the hardness you measure. |
| Working range | The researched temper range is 149–232°C / 300–450°F. Do not assume higher tempering always means higher toughness. |
The detail to pay attention to
A short forge heat on coarse spheroidised bar may leave carbon insufficiently dissolved. Repeating it hotter without understanding the starting condition is not a reliable fix. The normalise-and-quench forge route is a separate process.
If the coupon stays unexpectedly soft, write down the bar supplier and the actual hold before changing anything. Confirm the furnace reading and remove decarb from the measurement site. Do not add a stack of grain-refining cycles simply because a different maker uses them on another supply of steel.
Check the result before fitting the handle
Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.
Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.
Keep a record
Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.
After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.
Where this comes from
- How to Heat Treat 80CrV2, Knife Steel Nerds. Original experiments by metallurgist Larrin Thomas. Starting microstructure, hold and quench stay together. Do not transfer experimental property values to a different process.
- 80CrV2 tempering instructions, Alpha Knife Supply. Supports two 2-hour temper cycles only; hardening route above is KSN, not AKS’s different hardening temperatures.
Comments
Questions, corrections and what worked for you. Upvote comments you find useful.
Loading comments…