Learn / Heat treating

Heat treating 8670

If I wanted a knife that had to be tough, a big working blade for instance, 8670 is where I would look first. Testing found very high toughness and an easy heat treatment, which makes it a great choice for knives requiring high toughness and for beginning knifemakers and bladesmiths.

Knife Templates · 4 min read

Where I would start

A non-stainless nickel-chromium steel, so it rusts if it is left wet. It has high toughness and an easy heat treatment. The other side of that is wear resistance: it is relatively low, which means great ease in grinding, finishing and sharpening. Choose it for toughness, not for a long-lasting edge.

The recommended route for 8670 in a controlled furnace. The normalise and anneal below are for forged steel; bought annealed bar starts at the hardening heat. The test coupons were a standard quarter-size unnotched Charpy specimen.

Get the equipment ready

A controlled furnace, suitable surface protection for the hold, a commercial quench oil (Parks AAA, a slower oil, or a fast oil such as Parks 50) and a checked tempering oven.

Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.

A process to work from

Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.

8670: worked heat-treatment route
StageWhat to do
PrepareFinish the profile, holes and burr removal while soft. Leave measurable cleanup stock on the faces and edge.
Forged steel only: normalise and annealNormalise from 1550°F (843°C) for at least 10 minutes. Anneal by heating to 1380°F (749°C) for 30 minutes, cool at 500°F (278°C) an hour to below 1200°F (649°C), then air cool. Bought annealed bar skips this.
Austenitise1500°F (816°C) for 10 minutes. This is the tested sweet spot and the recommended heat treatment. As a general rule, stock thicker than 1/8″ (3.3 mm) may need a few more minutes.
QuenchFast or medium oil. 8670 has sufficient hardenability to use Parks AAA or even somewhat slower oils, and Parks 50 gives toughness just as good as AAA. Transfer promptly.
TemperBetween 300 and 450°F (149 to 232°C) depending on the hardness you want. Steel is typically tempered at least twice, 1 to 2 hours each, with air cooling between. No tempered martensite embrittlement showed at 450°F in the tests.

The detail to pay attention to

Do not read the headline toughness as what your blade will do. The 27.4 ft-lbs figure came from the best specimens and was higher than those in the rest of that study using the same steel. And overheating costs toughness for nothing: 1600-1625°F reduced toughness without an improvement in hardness.

Keep one offcut from the same bar with the same surface protection, and establish your furnace timing and quench on that coupon before the knife. Be cautious about quenching anything in water; the oil route here is the one that was tested.

Check the result before fitting the handle

Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.

Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.

Keep a record

Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.

After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.

Where this comes from

  • How to Heat Treat 8670, Knife Steel Nerds. Larrin Thomas’s tests of 8670 with his recommended route. Composition figures and most results are in images, so this site quotes only the text. No producer datasheet for 8670 was found.
Next upHeat treating D2D2: the equipment, hardening hold, quench, temper and details that are easy to miss.

Comments

Questions, corrections and what worked for you. Upvote comments you find useful.

Loading comments…

Knife Templates