Where I would start
A powder-metallurgy stainless knife steel balancing corrosion resistance, toughness and wear resistance. It still needs a grind suited to the knife, and abrasives capable of finishing it after hardening.
Annealed stock and the manufacturer’s 2050°F route, using plates. This example takes the no-cold-treatment branch; adding a cold step changes the response and needs its own recorded process.
Get the equipment ready
A furnace capable of holding 1121°C / 2050°F, foil or atmosphere protection rated for that heat, effective quench plates and a verified tempering oven.
Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.
A process to work from
Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.
| Stage | What to do |
|---|---|
| Preheat | 843–871°C / 1550–1600°F and equalise. |
| Austenitise | 1121°C / 2050°F for 20 minutes at temperature. Thick sections can require more time. |
| Quench | Plate quench to below 52°C / 125°F. The manufacturer permits several methods; this example uses plates. |
| Cold branch | No cold treatment in this worked route. If adding one, schedule it after the quench and before tempering; do not copy hardness values between branches. |
| Temper | 177°C / 350°F, at least 2 hours. Cool to hand warm between tempers, then repeat for at least 2 hours. |
The detail to pay attention to
The manufacturer warns that tempering above approximately 400°C / 750°F reduces corrosion resistance. Do not borrow a secondary-hardening temper from another tool steel. A higher hardening temperature also belongs with its own hold time and cold-treatment choice.
Measure the coupon before aiming at a particular HRC on the knife. Record foil handling, time out of the furnace and whether the quench actually reached the specified temperature. Keep the schedule at one setpoint while you establish repeatability, then change one variable at a time.
Check the result before fitting the handle
Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.
Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.
Keep a record
Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.
After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.
Where this comes from
- CPM MagnaCut datasheet, issue 1, March 2021, Crucible Industries. Page 2, including visual table. 2050°F corresponds to a 20-minute minimum hold. Manufacturer rounds C values; our conversions use the F setpoints. No-cold plate route kept separate from freezer and cryogenic branches.