Where I would start
A stainless steel sold by New Jersey Steel Baron and first released in 2017, designed with Buderus as a version of Uddeholm AEB-L modified with nitrogen and vanadium. The vanadium addition is very small, likely too small to contribute to wear resistance and edge retention.
The recommended route for Nitro-V: 15 minutes between 1900 and 1950°F, a plate quench and a cold treatment. The experiments used liquid nitrogen for an hour. The article does not say which AEB-L it compares against.
Get the equipment ready
A furnace holding 1900 to 1950°F (1038 to 1066°C), quench plates, liquid nitrogen (or at least a household freezer, used straight after the quench) and a checked tempering oven. The article does not cover surface protection for the hold, so use the foil guidance for stainless steel.
Measure the furnace and tempering oven independently where possible. A controller display is a setpoint, not proof that the whole blade has reached it. Timing a hold starts after equalisation, not as soon as the door closes.
A process to work from
Use this as a complete route to establish on a coupon from your stock. Temperatures in Celsius are rounded conversions of the Fahrenheit setpoints. A different supplier, section or starting condition can need a different process.
| Stage | What to do |
|---|---|
| Prepare | Finish the profile, holes and burr removal while soft. Leave measurable cleanup stock on the faces and edge. |
| Austenitise | 1900 to 1950°F (1038 to 1066°C) for 15 minutes. Peak hardness was reached at 1950°F and stayed flat to 2000°F, so the advice is to austenitise no higher than 1950°F. The extra heat does not buy strength: 2000°F likely leads to a decrease in strength and toughness. |
| Quench | Plate quench. It can be cooled in air or plate quenched for hardness. Oil quenching is also possible, though plate quenching helps maintain flatness. |
| Cold step | Liquid nitrogen straight after the quench; the experiments held it for an hour. Cryogenic processing is recommended for maximising strength. With a freezer instead, use 1900°F, and go into a household freezer directly after quenching at the very least. |
| Temper | 300 to 350°F (149 to 177°C) depending on the hardness you want. The toughness specimens were tempered twice at 350°F for two hours each time. Tempering higher than 350°F cannot be recommended right now. |
The detail to pay attention to
Do not temper to 450°F: the 450°F temper reduced hardness and toughness, so it is not recommended. That was unexpected, because tempered martensite embrittlement is not expected at this tempering temperature in high alloy steels, and it is not known whether 400°F behaves the same. Know what you have bought, too: in cold treatment tests, steel sold as AEB-L was Buderus X65Cr13 and needed higher austenitising temperatures. I found no producer datasheet for Nitro-V, so this route rests on one source.
Run a coupon through the whole route first, with the cold step straight after the quench. Edge retention and corrosion resistance are explicitly unconfirmed for this steel, so judge the finished knife in its own work rather than by the AEB-L comparison.
Check the result before fitting the handle
Clean scale and decarburisation from the test surface before interpreting a hardness reading. Use a flat, supported area and a calibrated method appropriate to the sample thickness. A file skating across a blade is a rough check, not an HRC measurement.
Inspect the tempered blade in good light for cracks, edge waves and distortion. If a blade is cracked, retire it. If hardness is unexpectedly low, check the whole record before increasing temperature or repeating a quench.
Keep a record
Keep the stock supplier and batch, blade and edge thickness, furnace program, actual hold, oil or plate details, cold-treatment branch and temper cycles beside the editable design. Add measured hardness and where it was measured.
After grinding and sharpening, evaluate the finished knife in its intended cutting work. Keep notes on edge stability, sharpening and geometry. Change one main variable so you can tell what helped as you learn.
Where this comes from
- Nitro-V: Its Properties and How to Heat Treat It, Knife Steel Nerds. Larrin Thomas’s tests of Nitro-V against AEB-L and 14C28N, with his heat treatment recommendation. The composition table is an image, so none is given here, and I found no producer datasheet. He says edge retention and corrosion resistance still need testing.
Comments
Questions, corrections and what worked for you. Upvote comments you find useful.